https://www.avient.com/sites/default/files/2022-09/Smartbatch Blow Molding Brochure.pdf
We’ll provide step-by-step guidance, and
visualization through in-house sampling
with various processing techniques:
• Injection stretch blow molding (ISBM)
• Extrusion blow molding (EBM) –
up to four layers
• Injection molding
Our polymer science proficiency, colorants and
additives capability, and in-house color design
service make us a powerful collaborator during
the complete blow molding process.
https://www.avient.com/sites/default/files/2023-04/Colorant Chromatics Transcend Healthcare Colorants Product Bulletin.pdf
Transcend Healthcare Colorants are available with
low minimum order quantities and full technical and
customer service support.
https://www.avient.com/sites/default/files/2025-06/LFT Brackets Application Bulletin.pdf
Complēt™ long glass, long carbon, and
hybrid fiber solutions available in a
wide array of engineering polymer
matrices, including PA66, PA6, ETPU,
PPA, PPS, PES, PEI, PK, and PEEK
• OnForce™ long glass fiber reinforced
polypropylenes
• Full suite of design and engineering
services that include structural design
and fiber orientation consultations and
modeling, CAE analysis, prototyping,
and more
STRENGTH-TO-WEIGHT RATIO OF LFT VS METALS
m
eg
ap
as
ca
l
gram
/cubic centim
eter
250
200
150
100
50
0
9.00
8.00
7.00
6.00
5.00
4.00
3.00
2.00
1.00
0.00
Zam
ak 3
Stainless Steel 304
Titanium
#2
plēt LCF40-PP
plēt LGF60-TPU
OnForce LGF50-PP
Alum
inum
A380
M
agnesium
AZ91D
plēt LCF50-PA66
plēt LGF60-PA66
plēt LCF50-TPU
Specific Strength Density
Metal
Long Glass Fiber
Long Carbon Fiber
1.844.4AVIENT
www.avient.com
Copyright © 2025, Avient Corporation.
https://www.avient.com/sites/default/files/2021-02/2021-baird-sustainability-conference.pdf
Microsoft PowerPoint - 2021 Baird Sustainability Conference
AVIENT CORPORATION
(NYSE: AVNT)
B A I R D
S U S T A I N A B I L I T Y
C O N F E R E N C E
F E B R U A R Y 2 3 , 2 0 2 1
WALTER RIPPLE
V I C E P R E S I D E N T , S U S T A I N A B I L T Y
• 28 Years Industry Experience
• Bachelors of Chemistry, Texas A&M University
• Executive MBA, University of Michigan
• Former VP & General Manager, Global GLS
TPE Business
• 2+ years Vice President, Sustainability
Avient Corporation 2
SUSTAINABILITY
A T A V I E N T
P E O P LE P RO D U CT S P LA N E T P E R F O RM AN CE
O U R M I S S I O N
E N A B L E O U R C U S T O M E R S ’ I N N O V A T I O N A N D S U S T A I N A B I L I T Y G O A L S
T H R O U G H W O R L D C L A S S P R O D U C T S A N D S E R V I C E S A N D E X C E L L E N C E I N
T H E F O U R C O R N E R S T O N E S O F :
Avient Corporation 3
Enable 100% of products manufactured for
packaging applications to be recyclable or
reusable.
https://www.avient.com/sites/default/files/2023-07/Avient_CodeConduct_2023_Portuguese.pdf
A nossa empresa se empenha para manter um padrão global coerente de conduta ética, ao mesmo
tempo em que respeita as culturas e as práticas de negócios dos países e comunidades locais com que interagimos.
Criamos uma empresa com uma
ótima dinâmica: uma empresa com alcance global e
uma visão clara.
Como uma empresa global com sede nos Estados
Unidos, as leis dos EUA, e as leis e regulamentos de
outros países em que fazemos negócios, aplicam-se às
nossas atividades.
https://www.avient.com/sites/default/files/2020-07/avient-abac-thai-200721.pdf
subject=
http://avient.ethicspoint.com
5
การอา้งองิดว่น: ส ิง่ท ีต่อ้งกระทำ�และหา้มกระทำ�ของ ABAC
ส ิง่ท ีต่อ้งกระทำ�
• ทราบวา่ Avient ห้ามการตดิสินบนและการทุจรติไม่วา่ในรปูแบบใด และไม่อนุญาตให้มีการจ่ายเงินคา่อำ�นวยความสะดวก
• มีความรูเ้ป็นอย่างดเีกี่ยวกับลักษณะที่มีผลใช้บังคบัของนโยบาย ABAC ของเรา และส่ือสารให้ผู้ ใตบ้ังคบับัญชาและบุคคลที่สามทราบ
• ตัง้คำ�ถาม หากนโยบายหรอืการกระทำ�ที่จำ�เป็นตอ้งดำ�เนินการน้ันไม่ชัดเจน
• รายงานการละเมิดหรอืการละเมิดที่ตอ้งสงสัยโดยทันทีตอ่ผู้บังคบับัญชาของคณุ ฝ่ายกฎหมาย หรอืสายดว่นจรยิธรรม
• ทราบวา่ “มูลคา่” ไม่จำ�เป็นตอ้งวดัเป็นตวัเงินเสมอไป
• ทราบวา่การตดิสินบนรวมถึงส่ิงตอ่ไปน้ี:
• เงินสดและส่ิงที่เทียบเท่าเงินสด (บัตรของขวญัหรอืบัตรกำ�นัล)
• ของขวญั ส่ิงบันเทิง และการเลีย้งรบัรองที่ ไม่มีวตัถุประสงคท์างธุรกิจที่ชัดเจน หรอืเกินความจำ�เป็นทางธุรกิจ
• การจ่ายเงินคา่เดนิทางหรอืการท่องเที่ยวพักผ่อน
• การจ่ายเงินให้กับเจ้าหน้าที่ของรฐัเพื่อให้ละเวน้ข้อกำ�หนดทางศลุกากรที่มีผลใช้บังคบัหรอืเพื่อเรง่รดัการจ่ายคนืภาษี
• การให้บรกิารส่วนบุคคล ความช่วยเหลือพิเศษ และเงินกู้ยืม
• การเสนอการจ้างงานหรอืผลประโยชน์อื่นให้กับสมาชิกในครอบครวัหรอืเพื่อนของบุคคลที่มีอิทธิพลน้ัน
• การให้เงินช่วยเหลือพรรคการเมืองหรอืผู้สมัครชิงตำ�แหน่งทางการเมือง
• การบรจิาคเงินหรอืการสนับสนุนทางการกุศล
• รายการอื่น ๆ ที่ ไม่ชัดเจนนัก ไดแ้ก่ การให้ความช่วยเหลือที่ ไม่ ใช่ตวัเงิน โอกาสในการลงทุน และการเอือ้หรอืให้ โอกาสสัญญารบัเหมาช่วง
• ทราบวา่ข้อห้ามน้ีมีผลใช้บังคบักับส่ิงใดก็ตามที่อาจเอือ้ประโยชน์ตอ่บุคคลโดยตรงหรอืตอ่บุคคลอื่น เช่น สมาชิกในครอบครวั เพื่อน หรอืผู้รว่มธุรกิจ
• รกัษาสมุดบัญชี บันทึก และบัญชีตา่ง ๆ ให้มีรายละเอียดที่สมเหตผุล และแสดงให้เห็นถึงการทำ�ธุรกรรมอย่างถูกตอ้งและเหมาะสม
• ทำ�การตรวจสอบวเิคราะห์สถานะของตวัแทน ผู้จัดจำ�หน่าย และบุคคลภายนอกอื่นทัง้ก่อนการทำ�สัญญาและระหวา่งความสัมพันธ์ทางธุรกิจ และขอรบัการอนุมัตจิาก
ฝ่ายกฎหมาย
• จัดการและตดิตามตรวจสอบกิจกรรมทางธุรกิจที่ดำ�เนินการผ่านบุคคลภายนอกอย่างเหมาะสม
ส ิง่ท ีต่อ้งไมก่ระทำ�
• เสนอ สัญญา จ่าย หรอือนุมัตกิารจ่ายส่ิงที่มีมูลคา่ใดก็ตามแก่เจ้าหน้าที่ของรฐัและ/หรอืพนักงานขององคก์รภาคเอกชน เพื่อช่วยให้ Avient ไดม้าซ่ึงหรอืการรกัษาไว้
ซ่ึงธุรกิจ หรอืรกัษาความไดเ้ปรยีบที่ ไม่เหมาะสมอื่นใดก็ตาม ข้อห้ามน้ีมีผลใช้บังคบัไม่วา่จะเป็นการเสนอหรอืการจ่ายที่ ไดก้ระทำ�โดยตรงหรอืผ่านบุคคลอื่นก็ตาม
• ป้อนข้อมูลที่บิดเบือนให้เข้าใจผิด ไม่ครบถ้วน หรอืเป็นเท็จลงในสมุดบัญชีและบันทึกของ Avient
• เพิกเฉยตอ่สัญญาณเตอืนอันตรายเมื่อรว่มธุรกิจกับบุคคลภายนอก
อเมรกิาเหนือ
Global Headquarters Avon Lake,
United States
33587 Walker Road Avon Lake,
OH, United States 44012
หมายเลขโทรฟร:ี 1-866-765-9663
โทรศัพท์: 1-440-930-1000
โทรสาร +440 930 3064
เอเชียแปซิฟิก
Regional Headquarters Shanghai,
China
2F, Block C 200 Jinsu Road
Pudong, 201206 Shanghai, China
โทรศัพท์: +86 (0) 21 6028 4888
โทรสาร +86 (0) 21 6028 4999
อเมรกิาใต ้
Regional Headquarters Sao Paulo,
Brazil
Av.
https://www.avient.com/sites/default/files/2022-11/Avient Announces Third Quarter 2022 Results.pdf
Adjusted EPS excluding intangible amortization for the third quarter of $0.59 was slightly below
prior year of $0.61.
2
“As we announced in our September 27th release, we are experiencing weaker global demand
conditions precipitated by the war in Ukraine, recession fears, higher energy costs and inflation,”
said Robert M.
Factors that could cause
actual results to differ materially from those implied by these forward-looking statements include,
but are not limited to: disruptions, uncertainty or volatility in the credit markets that could adversely
impact the availability of credit already arranged and the availability and cost of credit in the future;
the effect on foreign operations of currency fluctuations, tariffs and other political, economic and
regulatory risks; the current and potential future impact of the COVID-19 pandemic on our
business, results of operations, financial position or cash flows including, without limitation, any
supply chain and logistics issues; changes in laws and regulations regarding plastics in
jurisdictions where we conduct business; fluctuations in raw material prices, quality and supply,
and in energy prices and supply; production outages or material costs associated with scheduled
or unscheduled maintenance programs; unanticipated developments that could occur with
respect to contingencies such as litigation and environmental matters; our ability to achieve the
strategic and other objectives relating to the Avient Protective Materials business; an inability to
raise or sustain prices for products or services; our ability to pay regular quarterly cash dividends
and the amounts and timing of any future dividends; information systems failures and
cyberattacks; amounts for cash and non-cash charges related to restructuring plans that may
differ from original estimates, including because of timing changes associated with the underlying
actions; and other factors affecting our business beyond our control, including without limitation,
changes in the general economy, changes in interest rates, changes in the rate of inflation and
any recessionary conditions.
https://www.avient.com/sites/default/files/2020-10/luxury-closures-gravi-tech-design-guide-2.0-application-specific.pdf
Design Guide 25
CHAPTER 6 | TROUBLESHOOTING
FOUR MAIN AREAS
Check all of these areas before changing
anything in the process. 4
Mold
• Cooling channel obstructed
• Vent plugged
• Core bent
• Damaged tooling
• Runner shutoff partially closed
• Part stuck
• Gate plugged
• Tooling shifted
Machine or Equipment
• Thermolator unplugged
• Variac unplugged
• Material bridging
• Drying turned off
Material
• Contamination
• Lot change
• Poor mixing
• Material dust
• Material not dried
Process
• Changes
- Documented
- Undocumented
OBTAIN INFORMATION
Obtain as much information as possible about
the defect
• Ask operators
- When did it start occurring
- Is it on every part
• Set-Up Tech
- Is this how the process started up
- Has this happened before
STRATEGY THEORY
Part Consistency
• Does the defect happen randomly or
every part
Machine Cycle
• Is it consistent
• Injection pressure limited
• Screw hesitation
Check Settings
• What changed
• Did a heater band turn off
• Are valves sticking
Determine at which point in the process the
defect occurs
• Injection
• Hold time
• Gate frozen
• Ejection
• Part deforming due to ejection
• Do a short shot progression
Change ONE setting at a time, and allow time
for adjustment to affect the defect
• Change speeds and pressures first
- Take immediate effect and easily reversed
• Change temperatures last
- Take time to settle in
• Extreme Measures
- Put mold into different press
26 Gravi-Tech
Damages or worn
gate/sprue
Temperature settings
overriding or changed
Sprue breaks too soon
Lower viscosity lot
Nozzle too hot
Cooling time too low
Not enough
Reduce gate size
Increase cooling in
gate areas
Check gate for
blockages
Install a shorter nozzle or
specialty nozzle
Ensure nozzle is
temperature controlled
Dry material Add screw
Reduce nozzle tip
Angel Hair
• Commonly occurs on sprues and hot runner gates
• Long, thin strands of plastic material, which can tangle and cause components
to stick together
• Can cause ejection problems
Root cause: Gate or sprue is not frozen and draws molten material with the sprue/part during
mold open phase.
Note: Once the process has been established, the parts should be tested for dimensional stability over the range of service
termperatures.
https://www.avient.com/sites/default/files/2024-10/Avient_CodeConduct_2024_ES-LATAM2.pdf
Nuestras acciones,
productos y personas respaldan a
los países y comunidades globales
donde operamos”.
Lea nuestra Política global de gastos comerciales
que está disponible en The Loop, en People & Departments (Personal
y Departamentos), Ethics & Corporate Policies (Ética y Políticas
Corporativas).
Comercio internacional
Como empresa global, debemos cumplir con los controles y las
restricciones sobre la importación y exportación de las jurisdicciones
aplicables y las leyes de EE.
https://www.avient.com/sites/default/files/2023-06/Omnicolor Brochure.pdf
The range of world-
class services includes:
COLOR TECHNOLOGY
Custom matching, saturated colors &
special effects to fill market niches and
eliminate secondary operations.
COLOR AND DESIGN SERVICES
Trend and color insights, and product
development assistance to optimize
design and gain speed to market.
FIELD TECHNICAL SERVICE
Support for tool design, startup and
production optimization to gain
manufacturing efficiencies.