https://www.avient.com/sites/default/files/2020-09/edgetek-processing-guide.pdf
Base Resin PPA PC PSU PES PPS
Co-
polymer
Acetal
PEEK PA
Barrel Temperatures* °F (°C)
Rear Zone 550–580
(288–305)
550–590
(288–310)
600–640
(316–338)
630–660
(332–338)
550–580
(288–304)
350–370
(177–188)
660–700
(349–371)
440–490
(227–254)
Center Zone 560–600
(293–316)
570–600
(300–316)
620–670
(327–354)
650–680
(343–360)
560–615
(293–324)
380–390
(193–200)
700–730
(371–388)
470–510
(243–266)
Front Zone 580–620
(304–327)
580–630
(304–322)
630–680
(332–360)
670–730
(354–388)
590–630
(310–332)
390–430
(200–221)
720–750
(382–400)
490–540
(254–282)
Nozzle 575–615
(302–324)
580–630
(304–322)
630–680
(332–360)
680–700
(360–371)
600–625
(316–330)
380–415
(193–213)
720–750
(382–400)
520–570
(271–300)
Melt
Temperature
575–615
(302–324)
580–625
(304–330)
625–675
(330–358)
650–710
(343–377)
600–625
(316–330)
370–410
(188–210)
670–740
(354–393)
520–570
(271–300)
Mold
Temperature
250–300
(121–150)
175–240
(80–116)
190–300
(88–150)
225–325
(107–164)
250–325
(121–164)
190–250
(88–121)
290–375
(143–190)
150–200
(66–93)
Pack & Hold
Pressure
50%–75%
of Injection Pressure
Injection
Velocity
in/s
1.0–3.0
Back Pressure
psi 50
Screw Speed
rpm 50–90
Drying
Parameters
°F (°C)
6 hrs @ 175
(80)
4 hrs @ 250
(121)
4 hrs @ 275
(135)
4 hrs @ 250
(121)
3 hrs @ 300
(150)
2 hrs @ 200
(93)
3 hrs @ 275
(135)
4 hrs @ 180
(82)
Cushion
in 0.125–0.250
Screw
Compression
Ratio
2.5:1–3.5:1 2.0:1–2.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1
Nozzle
Type
General
General
General
General
General
General
General
Reverse
Taper
Clamp
Pressure 5–6 Tons/in2 of projected area of cavities and runner system
* Barrel temperatures should be elevated for compounds designed for electrical insulative properties.
Cut vent depths to:
- PPA Compounds: 0.0015"–0.0025" depth and 0.250" width
- PC Compounds: 0.002"–0.004" depth and 0.250" width
- PSU Compounds: 0.003"–0.004" depth and 0.250" width
- PES Compounds: 0.003"–0.004" depth and 0.250" width
- PPS Compounds: 0.002"–0.003" depth and 0.250" width
- Acetal Compounds: 0.0015" minimum depth and 0.250" width
- PEEK Compounds: 0.002"–0.004" depth and 0.250" width
- Nylon Compounds: 0.002" minimum depth and 0.250" width
• Increase vent depth to 0.060" (1.5mm) at 0.250" (4.0mm) away from the cavity
and vent to atmosphere.
https://www.avient.com/sites/default/files/2020-09/gravi-tech-processing-guide-chinese.pdf
基础树脂 加工指南 3 PC PE PEEK PP PPS 480–570 (250–300) 400–445 (200–230) 660–700 (350–475) 400–440 (200–225) 520–600 (270–300) 500–580 (260–305) 410–455 (207–237) 670–710 (357–385) 410–450 (205–230) 550–610 (285–310) 515–590 (267–310) 420–465 (213–243) 680–720 (363–400) 420–455 (215–235) 570–620 (300–320) 530–600 (275–315) 430–475 (220–250) 700–730 (370–395) 430–460 (220–240) 610–620 (320–325) 530–615 (275–325) 430–495 (220–260) 700–725 (370–385) 430–475 (220–250) 610–635 (320–335) 160–240 (70–115) 80–140 (25–60) 300–400 (150–200) 80–140 (25–60) 190–300 (90–150) 250 (125) 3–4 小时 0.02% 160 (70) 2 小时 2 小时 300 (150) 3–4 小时 0.10% 160 (70) 280 (135) 2–3 小时 0.01%–0.20% 备注 1.
通用 通用 通用 通用 通用 加工指南 3 PC PE PEEK PP PPS 480–570 (250–300) 400–445 (200–230) 660–700 (350–475) 400–440 (200–225) 520–600 (270–300) 500–580 (260–305) 410–455 (207–237) 670–710 (357–385) 410–450 (205–230) 550–610 (285–310) 515–590 (267–310) 420–465 (213–243) 680–720 (363–400) 420–455 (215–235) 570–620 (300–320) 530–600 (275–315) 430–475 (220–250) 700–730 (370–395) 430–460 (220–240) 610–620 (320–325) 530–615 (275–325) 430–495 (220–260) 700–725 (370–385) 430–475 (220–250) 610–635 (320–335) 160–240 (70–115) 80–140 (25–60) 300–400 (150–200) 80–140 (25–60) 190–300 (90–150) 250 (125) 3–4 小时 0.02% 160 (70) 2 小时 2 小时 300 (150) 3–4 小时 0.10% 160 (70) 280 (135) 2–3 小时 0.01%–0.20% 备注 1.
PC化合物:0.001"–0.002" 深,0.250" 宽 PC/PSU化合物:0.002"-0.003" 深,0.250" 宽 PES化合物:0.003"-0.004" 深,0.250" 宽 PEI化合物:0.001"-0.003" 深,0.250" 宽 PP化合物:0.001"-0.002" 深,0.250" 宽 ABS化合物:0.0015"-0.0025" 深,0.250" 宽 PEEK化合物:0.002"-0.004" 深,0.250" 宽 尼龙化合物:0.002"最小深度,0.250" 宽 将离模腔4.0mm(0.250")处的排气口深度增加到1.0mm(0.040"),并且 通向大气。
https://www.avient.com/sites/default/files/2020-11/controller-grip-case-study.pdf
Ultimately, the company selected a Versaflex™ OM
overmolding grade that bonded tightly to the
polycarbonate (PC) substrate of the grips without the
need for adhesives.
https://www.avient.com/sites/default/files/2022-09/Cesa Laser Marking Additives for Transportation Industry Bulletin.pdf
Cesa Laser Marking Additives can be used with
thermoplastics commonly used in vehicles
including:
• PP
• PC/ABS
• Polyamide
• Polyacetal (POM)
WHY SELECT LASER MARKING?
https://www.avient.com/sites/default/files/2023-05/Cesa Light Diffusion Additives for Automotive - Product Overview.pdf
We offer solutions for the
transparent and translucent thermoplastics used in
the automotive industry (typically PMMA and PC).
https://www.avient.com/sites/default/files/2023-10/Cesa Laser Additives Laser Welding Product Bulletin.pdf
waterproof
watches, and eyewear frames
• Healthcare products – ISO and USP pre-tested
solutions are sold as Mevopur™ Healthcare
Functional Additives
BENEFITS
• Produces strong, durable, and consistent seams
• Available for polyolefins, TPE, ABS, SAN, PA, PC,
PMMA, and others on request
• Delivered as concentrates or ready-to-use
formulations
• Can be combined with color into a single
product
• Specific regulatory compliance available on
request, e.g., UL 94 recognition, EU and US food
contact
• Product guidance from our experts
PRODUCT BULLETIN
Copyright © 2023, Avient Corporation.
https://www.avient.com/sites/default/files/2025-03/CAI Solutions for Recycled Resins in E_E Applications Product Bulletin _A4.pdf
Cesa™ Flame Retardant Additives enable a
fire performance in line with different levels
of Glow Wire temperatures (IEC 60685-2-12)
for various recycled resins including PP, PC,
and PS.
https://www.avient.com/resources/safety-data-sheets?page=1059
PPC750 PURPLE PC
PPC449 VENUS PC
PPC668 BLUE PC
https://www.avient.com/knowledge-base/article/overmolding-solutions?rtype[]=1164
Versaflex™ OM 1040X – Highly colorable solution for overmolding onto PC, ABS, and PC/ABS blends
Bonds to PC, ABS, PC/ABS, copolyester, and polystyrene
PC, ABS and PC/ABS overmolding materials are available in water-clear, natural, thin wall overmolding, and high performance grades.
https://www.avient.com/sites/default/files/2020-08/color-fabric-fx-product-bulletin-8.5x11.pdf
KEY CHARACTERISTICS
• Fabric FX can be formulated to include properties
such as UV color protection and anti-scratch
performance
• Fabric FX can be processed on standard molding
machinery
• Different matrix materials can be enhanced with
Fabric FX, including ABS, PC/ABS, PB, and unfilled
or talc-filled PP
• There is no limitation on the graining that can be
used; the fabric effect will differ depending on the
grain effect engraved in the tool
• If parts are extruded or a mold is not engraved,
final parts will have an attractive speckled
appearance, but will not be textured
TYPICAL USES
Fabric FX concentrates are suitable for any application
that could benefit from an enhanced textile-like
appearance.