https://www.avient.com/sites/default/files/2021-08/avient-korea-company-registrykor-21-08-04-5836551-v1.pdf
https://www.avient.com/knowledge-base/case-study/military-grade-protection-us-soldiers?rtype[]=1164
They are constructed from layers of 0°/90° woven E-glass fiber reinforcements combined with a proprietary resin system in a continuous pultrusion manufacturing process.
https://www.avient.com/knowledge-base/case-study/military-grade-protection-us-soldiers?ind[]=6595
They are constructed from layers of 0°/90° woven E-glass fiber reinforcements combined with a proprietary resin system in a continuous pultrusion manufacturing process.
https://www.avient.com/news/avient-specialty-inks-focuses-sustainability-debuts-updates-union-ink-branding-impressions-expo-2023
This includes unveiling a new logo for Union Ink, reimagining the established brand’s impressive portfolio of high-performing inks for 90 years with a new, modern look.
https://www.avient.com/news/avient-launches-medical-tpe-grades-formulated-without-animal-derivatives
Grades in the 60-90 Shore A durometer range can be used for IV connector caps, diagnostic testing devices, endoscopic caps, and similar applications.
https://www.avient.com/sites/default/files/2023-01/GlasArmor Ballistic Resistant Panels Case Study.pdf
Using GlasArmor panels, Ballisti-Wall® and Ballisti- Cover® solutions enable utility companies to add a superior level of protection to critical components and meet FERC security requirements within a modular, adaptable construction. 1 https://www.nbcnews.com/news/us-news/three-substations- attacked-washington-state-rcna63214 2 https://www.ferc.gov/sites/default/files/2020-04/E-4_10.pdf © 2023, All Rights Reserved Avient Corporation, 33587 Walker Road, Avon Lake, Ohio USA 44012 To learn more about Avient’s advanced composite solutions, visit www.avient.com/composites. https://www.nbcnews.com/news/us-news/three-substations-attacked-washington-state-rcna63214 https://www.nbcnews.com/news/us-news/three-substations-attacked-washington-state-rcna63214 https://www.ferc.gov/sites/default/files/2020-04/E-4_10.pdf http://www.avient.com/composites
https://www.avient.com/sites/default/files/2020-09/edgetek-processing-guide.pdf
Base Resin PPA PC PSU PES PPS Co- polymer Acetal PEEK PA Barrel Temperatures* °F (°C) Rear Zone 550–580 (288–305) 550–590 (288–310) 600–640 (316–338) 630–660 (332–338) 550–580 (288–304) 350–370 (177–188) 660–700 (349–371) 440–490 (227–254) Center Zone 560–600 (293–316) 570–600 (300–316) 620–670 (327–354) 650–680 (343–360) 560–615 (293–324) 380–390 (193–200) 700–730 (371–388) 470–510 (243–266) Front Zone 580–620 (304–327) 580–630 (304–322) 630–680 (332–360) 670–730 (354–388) 590–630 (310–332) 390–430 (200–221) 720–750 (382–400) 490–540 (254–282) Nozzle 575–615 (302–324) 580–630 (304–322) 630–680 (332–360) 680–700 (360–371) 600–625 (316–330) 380–415 (193–213) 720–750 (382–400) 520–570 (271–300) Melt Temperature 575–615 (302–324) 580–625 (304–330) 625–675 (330–358) 650–710 (343–377) 600–625 (316–330) 370–410 (188–210) 670–740 (354–393) 520–570 (271–300) Mold Temperature 250–300 (121–150) 175–240 (80–116) 190–300 (88–150) 225–325 (107–164) 250–325 (121–164) 190–250 (88–121) 290–375 (143–190) 150–200 (66–93) Pack & Hold Pressure 50%–75% of Injection Pressure Injection Velocity in/s 1.0–3.0 Back Pressure psi 50 Screw Speed rpm 50–90 Drying Parameters °F (°C) 6 hrs @ 175 (80) 4 hrs @ 250 (121) 4 hrs @ 275 (135) 4 hrs @ 250 (121) 3 hrs @ 300 (150) 2 hrs @ 200 (93) 3 hrs @ 275 (135) 4 hrs @ 180 (82) Cushion in 0.125–0.250 Screw Compression Ratio 2.5:1–3.5:1 2.0:1–2.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 2.5:1–3.5:1 Nozzle Type General Purpose General Purpose General Purpose General Purpose General Purpose General Purpose General Purpose Reverse Taper Clamp Pressure 5–6 Tons/in2 of projected area of cavities and runner system * Barrel temperatures should be elevated for compounds designed for electrical insulative properties.
Half-round runners are not recommended. • Only naturally balanced runner systems (“H” pattern) are recommended. • Runner diameters larger than 0.150" (3.8mm) and not exceeding 0.375" (9.5mm) are recommended. • Step each 90° bend in the system down in size (from sprue to gate) approximately 1/16" (1.5mm) to reduce pressure drop. • Place vents at each 90° intersection and vent to atmosphere. • Hot runner molds are acceptable and should be sized by the manufacturer.
Cold Slug Wells • Place these wells at the base of the sprue to capture the cold material first emerging from the nozzle. • Place wells at every 90° bend in the runner system. • Well depths approximately 1.5 times the diameter of the runner provide the best results.
https://www.avient.com/sites/default/files/resources/Lahnstein_ISO50001.pdf
Avient Colorants Germany GmbH Hohenrhein 1 56112 Lahnstein Germany Scope Production of Color Concentrates and Compounds Normative base ISO 50001:2018 Energy Management System Reg. no. 46089 Validity 17. 12. 2020 – 16. 12. 2023 Issue 12. 04. 2021 Swiss Made Swiss Association for Quality and Management Systems (SQS) Bernstrasse 103, 3052 Zollikofen, Switzerland sqs.ch F.
https://www.avient.com/sites/default/files/2021-08/20210802-certificate-of-incorporation.pdf
POLYONE SINGAPORE PTE LTD 12/04/2001 (Note: Only the five (5) most recent former names are listed.
https://www.avient.com/knowledge-base/article/injection-molding-mold-processing
75-
90°F
(25-
32°C)
When starting up a new mold, begin with short-shots, then gradually increase the shot size until all part cavities are 80-90% filled.
Maintain this speed until the part is 90% full and then reduce it further to completely fill the cavity without flashing the part.