https://www.avient.com/sites/default/files/2024-10/Avient_CodeConduct_2024_ES-SPAIN2.pdf
Lea nuestra Política global de gastos
empresariales disponible en The Loop, en People & Departments
(Personas y departamentos), Ethics & Corporate Policies (Ética y
políticas corporativas).
Puede encontrarlo en The Loop, en
People & Departments (Personas y departamentos), Ethics
& Corporate Policies (Ética y políticas corporativas).
La
Política de regalos y entretenimiento de Avient está disponible en The
Loop, en People & Departments (Personas y departamentos), Ethics &
Corporate Policies (Ética y Políticas corporativas).
https://www.avient.com/sites/default/files/2024-10/Avient_CodeConduct_2024_ZH-TW2.pdf
詳情載
於 The Loop 上的《全球隱私與資料保護政策》,位於「People &
Departments, Ethics & Corporate Policies」。
詳情載於 The Loop 上的《資訊系統使用政策》,位於「People &
Departments, Ethics & Corporate Policies」。
您可以在 The Loop 找到,位於「People & Departments,
Ethics & Corporate Policies」下。
https://www.avient.com/sites/default/files/2025-04/Supplier Code of Conduct FV_Spanish.pdf
Avient Corporation y sus subsidiarias y filiales ("Avient'') se comprometen a ser una
organización sostenible de categoría mundial.
https://www.avient.com/sites/default/files/2024-03/Nymax _ Nymax REC Processing Guide.pdf
Nozzle Drool
Nozzle temperature
too hot
• Decrease nozzle temperature
• Decrease back pressure
• Increase screw decompression
• Verify material has been dried at proper conditions
Incorrect nozzle • Use reverse taper tip
Weld Lines
Melt front
temperatures are
too low
• Increase pack and hold pressure
Mold design
• Increase gate size
• Perform short shots to determine fill pattern
and verify proper vent location
• Add vents and/or false ejector pin
• Move gate location
Warp
Process related
• Increase pack pressure
• Increase pack time
Mold design • Non-uniform mold cooling
Part design • Non-uniform wall thickness
Thermolator incorrect
temperature
• Check settings
• Inspect thermocouple
Processing Guide 7
Sticking in Mold
Overfilled cavity
• Decrease injection rate and pressure
• Decrease pack and hold pressure
• Adjust transfer position
• Decrease cooling time
Mold design • Increase draft angle
• Polish cores in direction of ejection
Part is too hot
1.844.4AVIENT
www.avient.com
Copyright © 2024, Avient Corporation.
https://www.avient.com/sites/default/files/2020-12/artisan-thermoplastics-nylon-processing-guide.pdf
Sink Marks
Melt too hot • Decrease nozzle and barrel temperatures
Insufficient
material volume
• Increase shot size
• Increase packing pressure
Part geometry
too thick
• Reduce wall thickness
• Reduce rib thickness
Processing Guide 5
Flash
Injection pressure
too high
• Decrease injection pressure
• Increase clamp pressure
• Increase transfer position
Excess
material volume
• Adjust transfer position
• Decrease pack pressure
• Decrease shot size
Melt or mold
too hot
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
Loose clamp • Reset mold height
• Increase clamp tonnage
Shrink
Too much shrink • Increase cooling time
Too little shrink • Decrease cooling time
Burning
• Reduce decompression
Mold design • Clean, widen and increase number of vents
• Increase gate size to reduce shear
Wet material • Verify material is dried at proper condition
Nozzle Drool
Nozzle temperature
too hot
• Decrease nozzle temperature
• Decrease back pressure
• Increase screw decompression
• Verify material has been dried at proper conditions
Incorrect nozzle • Use reverse taper tip
Weld Lines
Melt front
temperatures are
too low
• Increase pack and hold pressure
Mold design
• Increase gate size
• Identify end of fill pattern and verify proper
vent location
• Add vents or increase vent width
• Move gate location
6 Artisan Pre-Colored Thermoplastics
Warp
• Increase melt temp
• Reduce injection speed
• Increase pack pressure
• Increase pack time
• Decrease mold temperature
• Increase cool time
Mold design • Non-uniform mold cooling
Part design • Non-uniform wall thickness
Thermolator incorrect
temperature
• Check settings
• Inspect thermocouple
Sticking in Mold
Overfilled cavity
• Decrease injection rate and pressure
• Decrease hold pressure
• Decrease cooling time
Part too hot
• Decrease barrel temperature
• Decrease mold temperature
• Increase cooling time
Mold design • Increase draft angle
• Polish cores in direction of ejection
Black Specks
Contamination • Purge machine
Degradation
• Reduce melt temperature
• Reduce screw speed
• Reduce back pressure
Machine related • Check for wear on screw, barrel or check ring
Delamination
• Increase melt temperature
• Decrease injection speed
• Purge barrel to eliminate material contamination
Mold design • Reduce sharp corners in material flow path
• Increase venting
Processing Guide 7
Discoloration
Oversheared
material
• Decrease melt temperature
• Decrease injection speed
• Reduce residence time
Mold design • Increase gate sizing
Dry material • Check moisture of material to ensure it is within the
recommended moisture percentage for molding
1.844.4AVIENT
www.avient.com
Copyright © 2020, Avient Corporation.
https://www.avient.com/sites/default/files/2020-09/lubrione-processing-guide.pdf
Please contact Avient for processing conditions specific to your formulations.
1.844.4AVIENT
www.avient.com
Copyright © 2020, Avient Corporation.
https://www.avient.com/sites/default/files/2020-09/edgetek-processing-guide.pdf
PROBLEM CAUSE SOLUTION
Excessive Shrink Too much orientation • Increase packing time and pressure
• Increase hold pressure
• Decrease melt temperature
• Decrease mold temperature
• Decrease injection speed
• Decrease screw rpm
• Increase venting
• Increase cooling time
Not Enough Shrink Too little orientation • Decrease packing pressure and time
• Decrease hold pressure
• Increase melt temperature
• Increase mold temperature
• Increase injection speed
• Increase screw rpm
• Decrease cooling time
Burning Melt and/or mold
temperature too hot
Mold design
Moisture
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
• Clean, widen and increase number of vents
• Increase gate size or number of gates
• Verify material is dried at proper conditions
Nozzle Drool Nozzle temperature too hot • Decrease nozzle temperature
• Decrease back pressure
• Increase screw decompression
• Verify material has been dried at proper conditions
Weld Lines Melt front temperatures
too low
• Increase pack and hold pressure
• Increase melt temperature
• Increase vent width and locations
• Increase injection speed
• Decrease injection speed
• Increase gate size
• Perform short shots to determine fill pattern and verify
proper vent location
• Add vents and/or false ejector pin
• Move gate location
Warp Excessive orientation
• Increase cooling time
• Increase melt temperature
• Decrease injection pressure and injection speed
• Increase number of gates
Sticking in Mold Cavities are overpacked
Part is too hot
• Decrease injection speed and pressure
• Decrease pack and hold pressure
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
• Increase cooling time
• Increase draft angle
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
TROUBLESHOOTING RECOMMENDATIONS
PROBLEM CAUSE SOLUTION
Incomplete Fill Melt and/or mold
temperature too cold
Shot Size
• Increase nozzle and barrel temperatures
• Increase mold temperature
• Increase injection speed
• Increase pack and hold pressure
• Increase nozzle tip diameter
• Check thermocouples and heater bands
• Enlarge or widen vents and increase number of vents
• Check that vents are unplugged
• Check that gates are unplugged
• Enlarge gates and/or runners
• Perform short shots to determine fill pattern and verify
proper vent location
• Increase wall thickness to move gas trap
to parting line
• Increase cushion
Brittleness Melt temperature too low
Degraded/Overheated material
Gate location and/or size
• Increase melt temperature
• Increase injection speed
• Measure melt temperature with pyrometer
• Decrease melt temperature
• Decrease back pressure
• Use smaller barrel/excessive residence time
• Relocate gate to nonstress area
• Increase gate size to allow higher flow speed and lower
molded-in stress
Fibers on Surface
(Splay)
Melt temperature too low
Insufficient packing
• Increase melt temperature
• Increase mold temperature
• Increase injection speed
• Increase pack and hold pressure, and time
Sink Marks Part geometry too thick
Melt temperature too hot
Insufficient material volume
• Reduce wall thickness
• Reduce rib thickness
• Decrease nozzle and barrel temperatures
• Increase shot size
• Increase injection rate
• Increase packing pressure
Flash Injection pressure too high
Excess material volume
Melt and/or mold
temperature too hot
• Decrease injection pressure
• Increase clamp pressure
• Decrease injection speed
• Increase transfer position
• Decrease pack pressure
• Decrease shot size
• Decrease injection speed
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
• Decrease screw speed
TROUBLESHOOTING RECOMMENDATIONS
www.avient.com
Copyright © 2020, Avient Corporation.
https://www.avient.com/sites/default/files/2023-07/TPEs for Healthcare Industry Bulletin.pdf
REGULATORY
1.844.4AVIENT
www.avient.com
Copyright © 2023, Avient Corporation.
https://www.avient.com/sites/default/files/2025-04/Supplier Code of Conduct FV_Port.pdf
A Avient Corporation e as suas subsidiárias e afiliadas ("Avient") estão empenhadas
em ser uma organização sustentável e de classe mundial.
https://www.avient.com/sites/default/files/2021-09/supplier-code-of-conduct-es.pdf
Código de conducta para
proveedores de Avient
Avient Corporation y sus subsidiarias y filiales (“Avient”) se comprometen a ser una
organización sostenible de categoría mundial.